8 Defects in Hand Lay-Up FRP and Their Root-Cause Fixes

Oct 26,2026

Hand lay-up is forgiving to start and expensive to get wrong. Every one of the eight defects below has a root cause you can control before the resin is mixed, not after the part is demoulded.

Hand lay-up is forgiving to start and expensive to get wrong. Every one of the eight defects below has a root cause you can control before the resin is mixed, not after the part is demoulded.

Defect

Root cause

Fix

Blisters and voids

Air not rolled out; resin too viscous; poor wet-out; damp substrate

Roll every layer with a grooved roller; adjust viscosity; dry the reinforcement

Too much resin

Over-brushing to speed wet-out, pooling in corners

Lay flat first, then brush to a planned resin budget; spread pooled resin outward

Too little resin

Low thixotropy causing sag on vertical faces; wrong catalyst/promoter ratio

Raise thixotropy, speed gel, correct the dosing ratio

Discolouration / burn

Exothermic burn from thick single passes, or damp reinforcement

Keep each pass under 5 mm; reduce catalyst; lower shop temperature

Under-cure

Insufficient catalyst, poor mixing, water, trapped styrene, low temperature

Adjust catalyst to temperature, mix thoroughly, use dry cloth, ventilate

Contamination

Dirty cloth, dirty brushes, unclean floor

Clean reinforcement; keep gelcoat brushes separate from laminating brushes

Wrinkling, fuzzing, delamination

Fibre folds, cure too fast, poor wet-out, second layer laid after the first has cured

Lay up in time; stagger cut edges; keep adequate resin

Fibre show-through

Gelcoat too thin; laminated before gelcoat gelled; demoulded too early

Build gelcoat thickness; respect gel time before laminating

 

Two rules that prevent most of them

First, thickness per pass. Above about 5 mm in a single lay-up the exotherm burns the resin and discolours the part; above about 1.5 mm per coat in vinyl ester work the outside gels while the inside stays wet. Thin passes, controlled heat.

Second, environment. Keep relative humidity below 80% — moisture retards polyester and epoxy cure and can leave a permanently tacky surface. Keep the shop near 30 degrees C, and do not over-ventilate before gel, or you strip styrene out of the surface layer.

 

If you are using BPO, read this

Oxygen inhibition of the surface is noticeably stronger in benzoyl peroxide systems than in MEKP systems. If your shallow-coloured castings or patching compounds come out tacky, add around 0.02% wax to the surface resin or cover with film — do not simply increase the peroxide, which makes the exotherm worse without fixing the skin.

 

Repairing delamination properly

Cut out the full delaminated area and grind the surrounding sound laminate back at least 5 cm beyond the defect, then re-lay to the original specification. Patching only the visible edge leaves a stress concentrator and the defect returns.

Product pages: 

MEKP https://www.icasongroup.com/product_detail/1329848970192412672.html (laminating) 

BPO 50% paste https://www.icasongroup.com/product_detail/36.html (filler, putty, casting)

BPO 75% https://www.icasongroup.com/product_detail/101.html

 

Contact us

Talk to the ICASON peroxide team

Send us your resin system, process temperature, preferred product form and destination port. We reply with a grade recommendation, TDS/SDS, batch COA format and samples for qualified projects.

Tel: +86 16639328358

Whatsapp: +86 16639328358

Wechat: 166393238358

E-mail: icason001@icason.com

Website: www.icasongroup.com


Online Message

* Note: Please be sure to fill in the information accurately and keep the communication unblocked, we will get in touch with you as soon as possible

%{tishi_zhanwei}%