A pultrusion die at 150 °C and a hand lay-up shop at 25 °C are not looking for the same peroxide — yet both place the same order every month, and both complain about under-cure, runaway exotherm, or gel arriving before the fibres are wet out. In almost every case the initiator's decomposition speed was never matched to the process temperature.
1. What half-life measures
Half-life is the time for 50 % of the peroxide to decompose at a fixed temperature: t½ = 0.693 / kd, with kd following the Arrhenius equation [1]. Industry classifies every peroxide by the temperature at which its half-life reaches 10 h, 1 h and 0.1 h. The 10 h figure tells you where it starts to work; the 0.1 h figure tells you where it finishes fast [1].
2. Reference table (solution benchmarks)
| Grade | CAS | 10 h | 1 h | 0.1 h |
|---|---|---|---|---|
| LPO (dilauroyl peroxide) | 105-74-8 | 62 °C | 80 °C | 99 °C |
| BPO (dibenzoyl peroxide) | 94-36-0 | 73 °C | 92 °C | 113 °C |
| TBPEH | 3006-82-4 | 73 °C | 91 °C | 113 °C |
| TMCH | 6731-36-8 | 96 °C | 115 °C | 136 °C |
| TBEC | 34443-12-4 | 99 °C | 117 °C | 137 °C |
| DCP (dicumyl peroxide) | 80-43-3 | 115 °C | 135 °C | 157 °C |
| BPDH | 78-63-7 | 119 °C | 138 °C | 160 °C |
| BIBP | 25155-25-3 | 121 °C | 142 °C | 165 °C |
| DTBP | 110-05-4 | 126 °C | 146 °C | 168 °C |
3. Three bands
| Band | Window | Chemistry | Typical use |
|---|---|---|---|
| Low | 50–90 °C | Diacyl (LPO, BPO) | PVC polymerisation, acrylics, ambient UPR with accelerator |
| Medium | 100–140 °C | Peroxyketals, peresters (TMCH, TBEC, TBPEH) | SMC/BMC, pultrusion |
| High | 140–180 °C | Dialkyl (DCP, BPDH, BIBP, DTBP) | EPDM/silicone, XLPE, PP vis-breaking |
4. Reading it for your line
- Hand lay-up, 25 °C. BPO's 10 h temperature is 73 °C — far above ambient, which is exactly why ambient cure needs a cobalt or amine promoter to reach a controllable 10–45 min gel.
- Pultrusion die, 130–180 °C. Choose a 1 h half-life of 110–150 °C (TBPB, DCP). Blending a lower- and a higher-temperature grade widens the cure window and reduces shrinkage cracking in thick profiles.
- PP vis-breaking, 200–250 °C. Near-complete decomposition needs roughly 7–10 × the half-life at process temperature— check residence time before you check price.
Two caveats. These are solution benchmarks, so supplier gel-time data for your resin beats any chart. And batch-to-batch drift in active oxygen shifts gel time and peak exotherm, forcing constant line-speed correction — ask for historical COA data, not just the latest sheet.
5. Safety red line
Class 5.2 dangerous goods. Respect the SADT on the product documentation, keep peroxides away from accelerators, reducing agents and heavy-metal contamination, and maintain cold-chain storage where the grade requires it.
Why ICASON
Shanghai ICASON New Material Co., Ltd. has served the chemical and new-materials industries since 2014, exporting to 40+ countries. Our organic peroxides unit (manufacturing and services via Changzhou JOHO Chemical) covers all three bands above, with active oxygen verified on every COA.
- Overseas warehouse — operating in Turkey serving Russia, the Middle East, Eastern Europe and North Africa; further sites planned in the Netherlands, India, Vietnam, Mexico and Brazil
- 200+ laboratory-developed products; Class 5.2 compliant logistics
- Browse the range: Organic Peroxides
Tel / WhatsApp: +86 16639328358 | WeChat: 166393238358 E-mail: icason001@icason.com | www.icasongroup.com
Dosages are reference starting points. Confirm on a cup gel test at your own resin temperature, filler loading and part thickness before production.