How Much Texturing Agent Should You Actually Add? — Three Single-Variable Comparisons in One HAA System

Oct 21,2026

Who this is for: powder coating manufacturers — formulators currently running, or about to run, textured powder. The 60-second answer: the texturing agent controls texture coarseness, the leveling agent controls fineness — but the leveling agent also pushes gloss back up. These two variables are a seesaw. Never move only one of them. Data note: the comparison data below is quoted from published industry research (Fujian Wan'an Group, "Synthesis and Properties of HAA-Cured Polyester Resin for Textured Powder Coatings", republished by the "Powder on Stage" technical account). It is used here to illustrate dosage trends and is not our own test data. Validate on your own line before scaling.

 

1. Why Texture Stability Is So Hard to Hold

Textured powder is normally signed off on three things: texture coarseness, gloss, and scratch resistance. The first two are decided almost entirely by two variables:

  1. texturing agent dosage;
  2. leveling agent dosage.

The trouble is that these two interfere with each other. More texturing agent means coarser texture and falling gloss; more leveling agent means finer texture but gloss climbing back up. When a line produces texture that is "coarse one batch, fine the next", the root cause is very often that these two variables were never locked down together.

Below, two single-variable data sets from the published study — both in the same HAA system — put that seesaw in numbers.

 

2. Experimental Design (public, reproducible basis)

ItemCondition
Resin systemHAA-cured carboxyl-terminated polyester (acid value 28–34 mgKOH/g, Tg 60–65°C)
Cure schedule180°C × 15 min
Film thickness60–80 μm
Variable 1Texturing agent SA207: 0.10% / 0.15% / 0.20%
Variable 2Leveling agent GLP588: 0 / 0.40% / 0.80%
Other componentsSame resin lot, same filler lot; single-variable method

Note: HAA systems need a slightly higher extrusion temperature than conventional systems (about 115–120°C) to ensure the HAA disperses fully. This process prerequisite is frequently overlooked when running textures in an HAA system.

 

3. Variable 1: Texturing Agent Dosage → Gloss and Texture

Texturing agent dosageFilm gloss (60°)Texture and feel
0.10%13.1%–14.5%Fine texture, good overall performance
0.15%7.0%–7.2%Fine texture, good overall performance
0.20%5.2%–5.4%Slightly coarse texture, good overall performance

Three readings, three conclusions:

  1. 0.10% is already enough to raise a texture. The effective window is narrow — do not treat this additive with a "add a bit more to be safe" mindset.
  2. From 0.10% to 0.20%, gloss falls from ~14% to ~5%. Every step up in dosage almost halves the gloss. Your gloss target is, read backwards, your dosage ceiling.
  3. Texture coarseness rises monotonically with dosage. Want fine texture, go low; want coarse, go high. There is no magic middle number — only your target value.

 

4. Variable 2: Leveling Agent Dosage → Fineness and Gloss Recovery

Leveling agent dosageFilm gloss (60°)Texture appearance
0 (none)7.0%–7.2%Slightly coarse texture
0.40%7.7%–8.8%Fairly fine texture
0.80%11.8%–12.5%Fine texture

Three readings again:

  1. Leveling agent clearly improves texture fineness — it turns "slightly coarse" into "fine".
  2. The price is gloss. At 0.80%, gloss climbs from around 7% to around 12% — almost double.
  3. It does not destroy the texture. Even at 0.80% the texture is still there, just finer. Leveling agent and texturing agent are not mortal enemies; they are a ratio.

 

5. Turning Both Data Sets Into One "Texture Tuning Map"

Two worked examples (derived from the ranges above):

  • Fine texture at ≤8% target gloss: hold the leveling agent near 0.4% (gloss 7.7–8.8%), start the texturing agent at the 0.15% step.
  • Coarse texture at ≤6% target gloss: use no leveling agent or very little (≤0.2%), push the texturing agent up to the 0.20% step.

Note that this is a trend derivation, not a formulation. Your resin lot, filler oil absorption and extrusion parameters will all shift both curves.

 

6. Rollout Sequence for Powder Coating Plants

  1. Fix the acceptance criteria first: gloss band + texture coarseness + scratch resistance, written into your internal standard.
  2. Single-variable trial plates: change one variable at a time, run a dosage ladder on the same resin lot.
  3. Three-lot consistency: once a point is selected, run three consecutive lots; only scale when gel time and gloss spread between lots is acceptable.
  4. Log the batch drift of both numbers: the actual dosage of texturing agent and leveling agent must be fine-tuned as resin lots change. Do not skip retain-sample comparison.

 

7. How We Work with Powder Coating Plants: Our Customized Service

We manufacture texturing agents and leveling agents on our own lines, so the two variables in this article are exactly the two variables we can set for you.

1. Ladder sample sets built around your resin and your gloss target. Tell us your polyester's acid value and your target gloss, and we produce a matched ladder — usually three texturing-agent steps (0.10% / 0.15% / 0.20% equivalent) crossed with two leveling-agent levels — so you can map the seesaw on your own line rather than on someone else's data sheet.

2. We adjust particle size, not just the number on the bag. Texture too coarse at the dosage your gloss target allows? We shift the particle-size distribution of our physical texturing agent instead of asking you to accept a coarser texture. That is a production change we make in-house.

3. We tune the leveling agent carrier to your resin. Leveling agents carry on a resin, silica or barium sulfate carrier. If the carrier and your polyester do not get along, no dosage will fix the flow. We supply the same active substance on an alternative carrier so you can isolate the variable.

4. Custom grade filing under your specification. Once a combination works, we file it as your specification: particle-size band, active content, carrier, recommended dosage range. Reorders are produced against that file, so the tenth batch behaves like the first.

5. In-house QC and three-lot proof. Every lot is tested in our own laboratory and released against your specification; retention samples are kept. Before volume we ship three consecutive lots with gel-time data attached so drift is visible before it reaches your extruder.

6. Full documentation and private label packing. TDS, SDS and COA with every shipment — issued by our own QC, not copied from a third party. Package weight, bag printing and pallet configuration can carry your brand.

Send us: resin acid value, resin supplier/grade, target gloss band, target texture reference (photo or panel), cure schedule. We return: recommended grade, starting dosage pair, and a ladder sample set. Price on request, per specification.

 

Contact us

Talk to the ICASON peroxide team

Tel: +86 16639328358    Whatsapp: +86 16639328358       Wechat: 166393238358            E-mail: icason001@icason.com

Online Message

* Note: Please be sure to fill in the information accurately and keep the communication unblocked, we will get in touch with you as soon as possible

%{tishi_zhanwei}%