Powder Coating Additive Specification Quick Reference: TGIC / HAA / Leveling Agent / Gloss Enhancer / Texturing Agent — Parameters and Dosage Compared
Classification: Industry News
Oct 29,2026

What this is: a specification reference page for powder coating manufacturers — use it directly when comparing quotations, setting incoming acceptance criteria, or building your internal control file. Parameter basis: publicly accepted industry ranges. Always confirm against the TDS of the specific product and lot; lot quality is released against the specification we agree with you and certified by our own QC.
1. Five Products × 12 Fields
| Field | TGIC | HAA | Leveling agent | Gloss enhancer (701 type) | Texturing agent |
| English name | Triglycidyl isocyanurate | β-Hydroxyalkylamide (tetrakis(2-hydroxyethyl)adipamide) | Leveling agent (mainly acrylics) | Gloss enhancer (acrylic copolymer) | Texturing agent (physical / chemical) |
| CAS No. | 2451-62-9 | 6334-25-4 family | Mixture (no single CAS) | Mixture (no single CAS) | Depends on structure |
| Chemical type | Heterocyclic, three epoxy groups | Hydroxyalkylamide groups | Acrylic homopolymer/copolymer, silicone-modified | Acrylate–methyl methacrylate copolymer | Physical: amide-modified vinylidene fluoride polymer; chemical: metal-organic complex |
| Key index | EEW ≈ 100–110 g/eq | Hydroxyl value 78–82 g/eq; MW 320.38 | Active content ≈ 60% (common for domestic grades) | Softening point 95–125°C | Whiteness ≥90%; D50 25–38 μm (reference) |
| Appearance | White crystalline powder | White fine powder, odourless | Solid granule/powder (on carrier) | Solid resin | White / slightly yellow powder |
| Melting range | ≈ 90–110°C | 125–130°C | — (carrier system) | 95–125°C (softening point) | Physical type: relatively high melting point |
| Volatiles | Low (per producer standard) | ≤1.5% | — | — | Thermal weight loss ≤0.20% (150°C/2 h, reference) |
| Recommended dosage | Polyester:TGIC ≈ 93:7 (by weight) | ≈ 5%–6% of polyester | 0.8%–1.5% (on binder) | 1%–2% (on binder) | Internal 3.5%–5% (on resin) / post-add 0.2%–1.5% (on total formula) |
| Suitable systems | Carboxyl polyester (exterior) | Carboxyl polyester (HAA-dedicated grade) | All powder systems (check carrier) | Pairs with homopolymer leveling agents; reducible with copolymer types | All systems (indoor/exterior binders differ) |
| Typical cure | 180–200°C × 10–15 min | 180°C/15 min or 190°C/10–12 min | Follows the system | Follows the system | Follows the system |
| Typical application | Architectural aluminium profiles, exterior railings, appliances, automotive parts | Exterior weathering, appliances, markets requiring TGIC-free | High-gloss / matte topcoats | Gloss build and suppression of fine craters | Exterior railings, construction machinery, air-conditioner housings |
| Packing and storage | 25 kg bags; cool, dry, sealed | 25 kg bags; moisture-protected | 25 kg bags | 25 kg bags | 25 kg bags; moisture and pressure protected |
2. TGIC: The Reference Curing Agent for Exterior Systems

Key parameters
- CAS 2451-62-9 | three epoxy functional groups, reacts stoichiometrically with carboxyl polyester
- EEW ≈ 100–110 g/eq | melting range ≈ 90–110°C
- Ratio: polyester:TGIC ≈ 93:7 (for exterior polyester of acid value 30–38 mgKOH/g)
Reference formulation skeleton
| Component | Dosage | Note |
| Carboxyl polyester (acid value 30–38) | 92–94 | Exterior grade |
| TGIC | 6.5–8.0 | Calculated from EEW stoichiometry |
| Leveling agent | 0.8–1.2 | Reduces orange peel |
| Benzoin | 0.3–0.6 | 0.5+ recommended for thick film |
| Pigments and fillers | 30–60 | Adjusted for hiding power |
Process: twin-screw extrusion at 80–110°C melt mixing → chipping → grinding and sieving (180–200 mesh) → electrostatic spray → cure 180–200°C × 10–15 min
Safety: TGIC dust is irritating to skin and eyes. Wear a dust mask, protective gloves and goggles, and ensure forced ventilation at the workplace. Some export markets regulate TGIC — check the destination country's requirements before accepting an order.
3. HAA: The First Choice for a TGIC-Free Route
Key parameters
- N,N,N′,N′-tetrakis(2-hydroxyethyl)adipamide | MW 320.38
- Hydroxyl value 78–82 g/eq | melting range 125–130°C | volatiles ≤1.5%
- Dosage: ≈ 5%–6% of polyester (for acid value 30–35 polyester)
- Extrusion needs a slightly higher temperature: 115–120°C (for dispersion)
- Cure: 180°C/15 min or 190°C/10–12 min
HAA vs TGIC — six-dimension comparison
| Dimension | HAA | TGIC |
| Toxicity | Low toxicity, non-irritating to skin | Irritating; restricted in some markets |
| Environmental | Environmentally friendly; fits TGIC-free specifications | Regulatory controversy |
| Cure speed | Fast (low activation energy) | Conventional |
| Thick film | Releases water; pinhole risk on thick film | Good thick-film behaviour |
| Tribo gun | Inherent tribo-charging; suitable | Requires an added tribo additive |
| Cost | Relatively lower formulated cost | Depends on market |
Note: an HAA-dedicated polyester (acid value 30–35) is required. Switching from a TGIC system is changing the formulation, not changing a number.
4. Leveling Agent
- Active substances: acrylic homopolymers/copolymers, silicone-modified acrylates, polysiloxanes, hydrogenated castor oil, PVB
- Common solid carriers: epoxy resin (epoxy systems only), polyester, fumed silica
- Dosage: 0.8%–1.5% (on binder); use the upper limit with high oil-absorption pigments and fillers
- Cost of overdosing: storage stability and powder free-flow suffer
- Common misunderstanding: fine pinpoint craters are not always caused by too little leveling agent — insufficient gloss enhancer or polyester batch variation cause them too. Check those two first.
5. Gloss Enhancer
- Acrylate–methyl methacrylate copolymer , softening point 95–125°C
- Dosage: 1%–2% (on binder)
- Cost of overdosing: reduced impact resistance and flexibility (watch this closely for exterior railing and profile customers)
- Pairing rule: an acrylic homopolymer leveling agent system requires a gloss enhancer; a copolymer multifunctional system can use less or none
6. Texturing Agent
- Physical type (amide-modified vinylidene fluoride polymers / polyolefins): raises melt viscosity, textures via surface tension, highly predictable
- Chemical type (metal-organic complexes): participates in the cure and textures by shortening gel time; strong matting effect
- Dosage: internal 3.5%–5% (on resin) / post-add 0.2%–1.5% (on total formula)
- Effect rule: dosage ↑ → coarser texture, lower gloss; the resin's melt viscosity determines texture uniformity
- Three gloss levers: texturing agent dosage (primary) + leveling agent dosage (raises gloss) + filler type and level (secondary)
7. Acceptance and Compliance Notes for Powder Coating Plants
- Incoming acceptance should cover: reactive index (EEW / hydroxyl value), melting range, volatiles, within-lot consistency, and measured gel time in your own resin system;
- Three-lot consistency: run three consecutive lots and compare (gel time, gloss, texture, impact) before scaling;
- Complete documentation: TDS / SDS / COA with every lot, with lot quality certified by the producer's QC;
- Regulatory check: TGIC is restricted in some markets; HAA is the common TGIC-free route — follow the destination country and your customer's specification.
How We Work with Powder Coating Plants: Our Customized Service
Every field in the table above is a parameter we can set, because we make these products on our own lines.
1. We produce to your specification, not to a catalogue. EEW and melting range for TGIC, hydroxyl value and volatiles for HAA, active content and carrier for leveling agents, softening point for gloss enhancers, particle-size band for texturing agents — these are production parameters for us. Agree a band with us and we produce to it, under a specification filed in your name.
2. Consolidation across the five families. Rather than running five suppliers and five sets of paperwork, you can consolidate onto one specification file and one QC contact. Fewer variables to reconcile, and one party accountable when a number moves.
3. Reference formulations built around your resin. The skeleton in Section 2 is a starting point, not a product. Send us your polyester acid value and your target film build, and we return a starting formulation with the ratio calculated from your resin lot rather than from a generic table.
4. In-house laboratory testing and lot release. Every lot is tested in our own laboratory — reactive value, melting range, volatiles, gel time — and released against your specification. Retention samples are kept. We also test in your resin when you send it, and report gel time measured in your system.
5. Three-lot qualification as standard for any new grade. Before you scale, we ship three consecutive production lots with data attached, so drift is visible at the trial stage instead of at full production.
6. Export-ready documentation and packing. TDS, SDS and COA issued by our own QC with every shipment, plus transport classification and UN information where applicable. Standard packing is 25 kg bags; bag weight, print, label and pallet configuration can be set to your requirement, including private label.
7. Scheduled production for repeat grades. For grades you run regularly we book production slots and hold safety stock, so a repeat order is a release rather than a fresh negotiation.
Send us: the products you use, your resin grades, your acceptance criteria, and your destination market. We return: a specification sheet per product, starting dosages, and trial samples. Price on request, per specification